The iron–carbon phase diagram is a foundation of steel metallurgy. It explains the stability of ferrite, austenite and cementite; the formation of pearlite; and the peritectic, eutectic and eutectoid reactions. It also provides a starting point for understanding annealing, normalising, hardening, tempering, casting and hot rolling.

MetaTechX Editorial · 11 Nov 2026 · 35 views
IRON–CARBON PHASE DIAGRAM

METATECHX ENGINEERS

AN IN-DEPTH GUIDE TO THE
IRON–CARBON PHASE DIAGRAM

Phases • Transformations • Microstructures • Heat Treatment • Steelmaking Applications


Technical learning document | Prepared by MetaTechX LLP

 

Executive Summary

The iron–carbon phase diagram is one of the most important tools in ferrous metallurgy. It shows the equilibrium phases that can exist in iron–carbon alloys as a function of carbon content and temperature. Engineers use it to understand solidification, austenitising, ferrite and cementite formation, eutectoid transformation, and the foundations of heat treatment.

The diagram most commonly used for steels is the metastable iron–iron carbide (Fe–Fe₃C) diagram. It is called metastable because cementite is not the ultimate equilibrium form of carbon; under suitable conditions graphite is more stable. The Fe–Fe₃C diagram is nevertheless extremely useful for ordinary steels and many cast irons because cementite-containing structures are commonly encountered in practical processing.

 

1. What Is the Iron–Carbon Diagram?

The iron–carbon diagram is a temperature-versus-composition map. The horizontal axis represents carbon content, normally in weight percent (wt.% C), and the vertical axis represents temperature in degrees Celsius. Each region indicates a phase or combination of phases that is stable at equilibrium for that composition and temperature.

The diagram is not a production recipe and does not directly show how quickly transformations occur. It describes equilibrium or near-equilibrium phase relationships. Actual plant cooling rates, alloying elements, section thickness and prior processing can shift transformation behaviour.

 

·       Steel range: conventionally up to about 2.11 wt.% carbon in the Fe–Fe₃C diagram.

·       Cast-iron range: above about 2.11 wt.% carbon up to the cementite composition at 6.67 wt.% C.

·       The diagram is commonly plotted up to 6.67 wt.% C because Fe₃C contains 6.67 wt.% carbon by mass.

 

 

2. Important Reference Points

Point / feature

Approximate value

Metallurgical significance

Pure iron melting point

1538°C

Liquid iron solidifies to δ-ferrite at the melting point.

δ ↔ γ transformation

About 1394°C for pure Fe

High-temperature BCC delta ferrite changes to FCC austenite on cooling.

γ ↔ α transformation

About 912°C for pure Fe

FCC austenite changes to BCC ferrite in pure iron.

Peritectic reaction

About 0.16 wt.% C and 1493°C

Liquid + δ-ferrite → austenite (γ).

Eutectic reaction

4.3 wt.% C and 1147°C

Liquid → austenite + cementite; forms ledeburitic structure.

Eutectoid reaction

About 0.76–0.77 wt.% C and 727°C

Austenite → ferrite + cementite; forms pearlite under near-equilibrium cooling.

Maximum carbon solubility in α-ferrite

About 0.022 wt.% at 727°C

Very limited carbon solubility in ferrite.

Maximum carbon solubility in γ-austenite

About 2.11 wt.% at 1147°C

Austenite can dissolve much more carbon than ferrite.

Cementite composition

6.67 wt.% C

Fe₃C is iron carbide, a hard and brittle compound.

 

Values are conventional approximate values used for engineering education. Exact diagram coordinates may vary slightly among published assessments and depending on the selected diagram.

 

3. Phases in the Iron–Carbon System

3.1 Ferrite (α-iron)

Ferrite is a body-centred cubic (BCC) form of iron that is stable at lower temperatures in the pure-iron system. It is relatively soft, ductile and tough, and it has very low carbon solubility. Its maximum carbon solubility is approximately 0.022 wt.% at the eutectoid temperature of 727°C; at room temperature it is much lower.

·       Low hardness and relatively low strength compared with pearlite or martensite.

·       Good ductility and formability, which is important in sheet, strip and drawing applications.

·       Magnetic below the Curie temperature (about 770°C); the magnetic change is not itself a crystal-structure transformation.

·       In low-carbon steels, ferrite is commonly the major constituent and contributes to softness and weldability.

3.2 Austenite (γ-iron)

Austenite has a face-centred cubic (FCC) crystal structure. Its interstitial spaces allow it to dissolve substantially more carbon than ferrite. In the metastable Fe–Fe₃C diagram, its maximum carbon solubility is about 2.11 wt.% at 1147°C.

·       Austenite is generally non-magnetic in the ordinary steel-processing temperature range.

·       It is the parent phase from which ferrite, pearlite, bainite or martensite may form during cooling, depending on composition and cooling history.

·       Austenitising is a key step in many heat-treatment operations, including normalising, hardening and some annealing processes.

·       Austenite stability and transformation temperatures are strongly influenced by alloying elements such as Mn, Ni, Cr, Mo and Si.

3.3 Cementite (Fe₃C)

Cementite is iron carbide with approximately 6.67 wt.% carbon. It is hard and brittle and contributes strongly to hardness, wear resistance and strength when present as fine particles or lamellae. Coarse or continuous cementite networks can reduce toughness and promote cracking.

·       Cementite is a metastable carbide in the Fe–Fe₃C diagram.

·       It may appear as lamellae in pearlite, as proeutectoid cementite in high-carbon hypereutectoid steel, or in other carbide morphologies.

·       Its size, distribution and continuity are as important as its total fraction for mechanical performance.

 

4. Other Important Phases and Microconstituents

Name

Description

Typical significance

δ-ferrite

High-temperature BCC iron phase near the melting range.

Relevant to solidification and high-temperature phase transformations.

Pearlite

Lamellar mixture of ferrite and cementite formed by eutectoid decomposition of austenite.

Provides a useful balance of strength and ductility; finer pearlite is generally stronger/harder.

Bainite

Non-equilibrium transformation product containing ferrite and carbide constituents, with morphology depending on temperature and alloy.

Can provide high strength with useful toughness.

Martensite

Supersaturated, diffusionless transformation product formed when austenite is cooled rapidly enough.

Very hard and strong; often requires tempering to improve toughness.

Ledeburite

Eutectic constituent of austenite and cementite formed at about 4.3 wt.% C and 1147°C.

Important in white cast irons; transforms further on cooling.

 

Pearlite, bainite and martensite are microstructures or transformation products rather than single equilibrium phases in the same sense as ferrite, austenite and cementite.

 

5. The Three Major Invariant Reactions

5.1 Peritectic Reaction

Liquid + δ-ferrite  →  Austenite (γ)

The peritectic reaction occurs at approximately 1493°C near 0.16 wt.% carbon. It is important in the solidification of low-carbon steels. In continuous casting, peritectic steel grades can exhibit distinctive solidification shrinkage and shell behaviour, making mould-powder selection, cooling and casting practice particularly important.

5.2 Eutectic Reaction

Liquid  →  Austenite (γ) + Cementite (Fe₃C)

The eutectic point is approximately 4.3 wt.% carbon at 1147°C. The eutectic constituent is called ledeburite. This reaction is especially important in cast irons and is outside the normal carbon range of most steels.

5.3 Eutectoid Reaction

Austenite (γ)  →  Ferrite (α) + Cementite (Fe₃C)

The eutectoid point is approximately 0.76–0.77 wt.% carbon at 727°C. The lamellar ferrite-cementite product is pearlite. This reaction is central to understanding the microstructure of plain-carbon steels.

 

6. How to Classify Steels by Carbon Content

Steel category

Carbon range (approx.)

Expected equilibrium transformation behaviour

Hypoeutectoid steel

Below 0.76–0.77 wt.% C

Proeutectoid ferrite forms first from austenite; remaining austenite transforms to pearlite at the eutectoid temperature.

Eutectoid steel

About 0.76–0.77 wt.% C

Austenite transforms predominantly to pearlite at the eutectoid temperature.

Hypereutectoid steel

Above 0.76–0.77 and up to about 2.11 wt.% C

Proeutectoid cementite forms first; remaining austenite transforms to pearlite at the eutectoid temperature.

 

The term proeutectoid means the constituent that forms from austenite before the remaining austenite reaches the eutectoid transformation temperature.

 

 

 

7. What Happens During Slow Cooling?

7.1 Hypoeutectoid steel — example 0.20 wt.% C

1.          At sufficiently high temperature, the steel is fully austenitic (γ), provided it is within the austenite field.

2.          On cooling below the A₃ boundary, ferrite begins to form along prior-austenite grain boundaries.

3.          Because ferrite rejects most carbon, the remaining austenite becomes progressively richer in carbon.

4.          At approximately 727°C, the remaining austenite transforms into pearlite.

5.          The final near-equilibrium structure is proeutectoid ferrite plus pearlite.

7.2 Eutectoid steel — example 0.77 wt.% C

If austenitised and cooled slowly under near-equilibrium conditions, the austenite transforms at about 727°C into pearlite. The final structure is predominantly pearlite, with no proeutectoid ferrite or cementite expected for the ideal eutectoid composition.

7.3 Hypereutectoid steel — example 1.0 wt.% C

6.          At high temperature in the austenite field, carbon is dissolved in γ-iron.

7.          On cooling below the Acm boundary, proeutectoid cementite begins to form, often at prior-austenite grain boundaries.

8.          The remaining austenite becomes leaner in carbon as cementite forms.

9.          At approximately 727°C, the remaining austenite transforms into pearlite.

10.     The final near-equilibrium structure is proeutectoid cementite plus pearlite.

 

8. Understanding the A₁, A₃ and Acm Lines

Line

Meaning in the Fe–Fe₃C diagram

Practical interpretation

A₁

Eutectoid temperature, approximately 727°C.

Below A₁, austenite is not an equilibrium phase in plain-carbon steel.

A₃

Boundary between the austenite field and austenite + ferrite field on the hypoeutectoid side.

On cooling, proeutectoid ferrite begins to form when crossing below A₃.

Acm

Boundary between the austenite field and austenite + cementite field on the hypereutectoid side.

On cooling, proeutectoid cementite begins to form when crossing below Acm.

 

In practical heating and cooling, engineers often use Ac₁, Ac₃ and Ar₁/Ar₃ notation to distinguish measured heating and cooling transformation temperatures. These can differ from equilibrium values because transformations require time and may show thermal hysteresis.

 

9. Lever Rule: Estimating Phase Fractions

The lever rule estimates the relative amounts of phases in a two-phase equilibrium region. It uses the horizontal tie-line at the temperature of interest and the compositions at the ends of that tie-line.

Fraction of phase 1 = (C₂ − C₀) / (C₂ − C₁)

Fraction of phase 2 = (C₀ − C₁) / (C₂ − C₁)

Here C₀ is the overall alloy carbon content, while C₁ and C₂ are the carbon concentrations at the two phase boundaries at the selected temperature. The fractions are mass fractions when compositions are expressed in weight percent.

Illustrative eutectoid example: just above 727°C, a 0.40 wt.% C steel lies in the α + γ region. Using the approximate tie-line endpoints of 0.022 wt.% C in ferrite and 0.76 wt.% C in austenite, the lever rule can estimate the ferrite and austenite fractions immediately above the eutectoid temperature. The remaining austenite then transforms to pearlite during slow cooling.

 

10. Relationship Between the Diagram and Heat Treatment

Heat-treatment process

Typical thermal approach

Microstructure / purpose

Full annealing

Heat into the austenite region as appropriate, soak, then cool slowly in the furnace.

Promotes a relatively soft, ductile structure and improves machinability or relieves processing effects.

Normalising

Heat into the austenite region, soak, then cool in still air.

Usually produces finer ferrite-pearlite than full annealing and refines the structure.

Hardening / quenching

Austenitise, then cool rapidly in a suitable quench medium.

Can form martensite; hardness depends on carbon, alloying, section size and cooling severity.

Tempering

Reheat quenched steel below A₁ for a controlled time, then cool.

Reduces brittleness and adjusts strength/toughness through tempering reactions.

Spheroidising

Long hold near or below A₁, often with controlled thermal cycling.

Produces rounded carbide particles in ferrite; improves machinability and cold formability of high-carbon steels.

 

The phase diagram helps select austenitising ranges and understand equilibrium transformations, but it does not by itself specify quench severity, holding time or final hardness.

 

11. What the Iron–Carbon Diagram Cannot Tell You

The equilibrium diagram is essential, but it has important limitations:

·       It does not show transformation time. It cannot predict whether pearlite, bainite or martensite will form at a particular cooling rate.

·       It does not provide hardenability. Hardenability depends on composition, grain size, section dimensions and cooling conditions.

·       It does not fully describe alloy steels. Elements such as Mn, Cr, Ni, Mo, Si, V, Nb and Ti shift transformation boundaries and form additional phases/carbides.

·       It does not describe segregation, dendritic solidification, inclusion behaviour or casting defects.

·       It does not predict the effect of deformation during rolling, recrystallisation or thermomechanical processing.

For these questions, engineers use Time-Temperature-Transformation (TTT) diagrams, Continuous-Cooling-Transformation (CCT) diagrams, thermodynamic databases, dilatometry and metallographic examination.

 

12. Application in Steelmaking and Rolling Mills

12.1 Steel composition control

Carbon content strongly influences the balance between strength, hardness, ductility and weldability. The phase diagram provides the foundation for understanding why a change in carbon content changes the proportions of ferrite, pearlite and carbide-containing constituents after cooling.

12.2 Reheating and hot rolling

Billets and slabs are reheated to temperatures selected for the steel grade and rolling schedule. The objective is to obtain a suitable austenitic condition, promote temperature uniformity and enable controlled deformation. Actual reheating practice must also consider oxidation, decarburisation, grain growth, alloy dissolution and surface quality.

12.3 TMT reinforcement bars

In thermomechanically treated (TMT) bars, the surface is rapidly quenched after rolling to create a hard transformed outer layer, while the core remains hotter and later self-tempers the surface. The final structure commonly contains a tempered martensitic rim and a ferrite-pearlite core, depending on grade, bar size, water-box design and process conditions. The equilibrium Fe–Fe₃C diagram gives background on austenite and carbon effects, but TMT design also requires CCT data, transformation kinetics, heat-transfer calculations and process trials.

 

12.4 ERW tube manufacturing

In ERW tube production, strip edges are heated and forged together to form a weld. The base-metal and weld-zone microstructures depend on steel chemistry, edge heating, squeeze pressure, upset removal, sizing and any subsequent heat treatment. The phase diagram supports understanding of the base steel, while weld thermal-cycle analysis and metallography are needed to assess the weld and heat-affected zone.

12.5 Casting and continuous casting

The liquidus, solidus and peritectic regions influence solidification behaviour. Peritectic grades may be sensitive to shell contraction and mould heat transfer. Casting engineers therefore combine phase-diagram knowledge with grade-specific solidification models, secondary cooling practice and mould-powder control.

13. Practical Metallurgical Examples

Example steel

Carbon content (illustrative)

Slow-cooled equilibrium expectation

Low-carbon structural steel

0.15–0.20 wt.% C

Ferrite-rich structure with a smaller pearlite fraction.

Medium-carbon steel

0.35–0.45 wt.% C

Ferrite plus pearlite; higher pearlite fraction than low-carbon steel.

Eutectoid plain-carbon steel

≈0.76–0.77 wt.% C

Predominantly pearlite.

High-carbon steel

0.90–1.00 wt.% C

Pearlite plus proeutectoid cementite under near-equilibrium cooling.

 

These are simplified examples. Commercial grades contain other elements, and actual microstructures depend on processing and cooling history.

14. How to Read the Diagram in Practice

11.     Locate the steel's carbon content on the horizontal axis.

12.     Locate the process temperature on the vertical axis.

13.     Identify the phase field at the intersection of composition and temperature.

14.     During cooling, follow the vertical composition line downward and note each boundary crossed.

15.     At a two-phase temperature, draw a horizontal tie-line and use the lever rule if phase fractions are required.

16.     Check whether the process is close to equilibrium. If cooling is rapid or deformation is significant, use CCT/TTT data and process-specific models.

 

Conclusion

The iron–carbon phase diagram is a foundation of steel metallurgy. It explains the stability of ferrite, austenite and cementite; the formation of pearlite; and the peritectic, eutectic and eutectoid reactions. It also provides a starting point for understanding annealing, normalising, hardening, tempering, casting and hot rolling.

For industrial engineers, the key is to use the diagram together with the real process history. Temperature, time, cooling rate, alloying elements, deformation and section size determine the microstructure that is actually produced. Combining phase-diagram knowledge with TTT/CCT diagrams, process control and metallography allows steel manufacturers to design reliable products with the required strength, ductility, toughness and wear resistance.

 

References and Further Reading

·       ASM Handbook, Volume 1: Properties and Selection: Irons, Steels, and High-Performance Alloys. ASM International.

·       ASM Handbook, Volume 4A: Steel Heat Treating Fundamentals and Processes. ASM International.

·       Callister, W. D. and Rethwisch, D. G., Materials Science and Engineering: An Introduction. Wiley.

·       Porter, D. A., Easterling, K. E. and Sherif, M. Y., Phase Transformations in Metals and Alloys. CRC Press.

 

Comments 0

Be the first to share your thoughts.

Leave a comment

Your comment will appear after a quick moderation check.

META TECHX GETCERTIFIED

Turn technical knowledge into verified proof.

Assess practical competency and earn a verifiable professional credential.

GetCertified →